Molecular engram polymer of pyrethroid-like pesticide and application thereof
A pyrethroid, molecular imprinting technology, applied in the direction of material separation, analysis of materials, instruments, etc., to achieve the effect of strong operability, high enrichment and good selectivity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] Example 1: Preparation of a molecularly imprinted polymer with cypermethrin as a template.
[0033] Weigh 1.0 mmol of the template molecule cypermethrin and add it into a glass test tube filled with 10 mL of toluene, and then add 6.0 mmol of α-methacrylic acid (MAA). The above reaction solution was placed in a high-power ultrasonic cleaner for ultrasonic treatment for 1 hour so that the cypermethrin pesticide molecule was fully combined with α-methacrylic acid, and then 30mmol of ethylene glycol dimethacrylate (EDMGA) was added as a crosslinking agent and 65mg of azobisisobutyronitrile (AIBN), then ultrasonic treatment for 10 minutes, and nitrogen gas (N 2 ) deoxygenated for 15 minutes, and finally vacuum-sealed. After the sealed glass test tube was placed in a 55° C. water bath thermostat to react for 48 hours, a block-shaped cypermethrin molecularly imprinted polymer was obtained. The molecularly imprinted polymer is ground and pulverized and passed through a 100-me...
Embodiment 2
[0035] Example 2: Preparation of a molecularly imprinted polymer with bifenthrin as a template.
[0036] Weigh 1.0 mmol of the template molecule bifenthrin and add it into a glass test tube filled with 10 mL of toluene, and then add 6.0 mmol of α-methacrylic acid (MAA). The above reaction solution was placed in a high-power ultrasonic cleaner for ultrasonic treatment for 1 hour, so that the bifenthrin pesticide molecules could fully interact with α-methacrylic acid, and then add 30 mmol of ethylene glycol dimethacrylate (EDMGA) to Combined agent and 65mg azobisisobutyronitrile (AIBN), then ultrasonic treatment for 10 minutes, and nitrogen gas (N 2 ) deoxygenated for 15 minutes, and finally vacuum-sealed. After the sealed glass test tube was placed in a 55°C water bath thermostat for 48 hours of reaction, a block-shaped bifenthrin molecularly imprinted polymer was obtained. The molecularly imprinted polymer is ground and pulverized and passed through a 100-mesh sieve and a 20...
Embodiment 3
[0038] Example 3: Preparation of a molecularly imprinted polymer with phenthrin as a template.
[0039] Weigh 1.0 mmol of the template molecule phenothrin and add it into a glass test tube filled with 10 mL of toluene, and then add 6.0 mmol of α-methacrylic acid (MAA). The above-mentioned reaction solution was placed in a high-power ultrasonic cleaner for ultrasonic treatment for 1 hour, so that the phenothrin pesticide molecule was fully combined with α-methacrylic acid, and then 30 mmol of ethylene glycol dimethacrylate (EDMGA) was added for the cross-linking process. Combined agent and 65mg azobisisobutyronitrile (AIBN), then ultrasonic treatment for 10 minutes, and nitrogen gas (N 2 ) deoxygenated for 15 minutes, and finally vacuum-sealed. After the sealed glass test tube was placed in a 55°C water-bath thermostat for 48 hours of reaction, a block-shaped molecularly imprinted polymer of phenthrin could be obtained. The molecularly imprinted polymer is ground and pulveriz...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com