Preparation method of sewing thread
A sewing thread and graphene technology, applied in the direction of conductive/antistatic filament manufacturing, conjugated artificial filament, fiber chemical characteristics, etc., can solve problems such as inappropriateness, achieve good antistatic performance, good application prospects, thickness uniform effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] This embodiment relates to a preparation method of sewing thread;
[0033] The preparation method of described sewing thread, comprises the steps:
[0034] (1) Prepare the following components by weight according to the following ratio:
[0035] 38 parts of polypropylene, 5 parts of polyethylene, 7 parts of polyvinyl alcohol, 10 parts of polyacrylamide, 1.2 parts of graphene, 4 parts of bamboo charcoal fiber, 3 parts of additives, 2 parts of emulsifier, 3 parts of additives;
[0036] (2) Weigh the proportioned amount of polyacrylamide and polyvinyl alcohol into the reaction kettle, raise the temperature to 60°C, slowly add graphene, and react at constant temperature for 2 hours to obtain the reaction product a1;
[0037] (3) Weigh the proportioned amount of polypropylene, polyethylene, bamboo charcoal fiber, emulsifier and reaction product a1 and place them in a banbury mixer for 20 minutes of banburying, pulverize the banbury-mixed products, and mix them evenly with a...
Embodiment 2
[0048] This embodiment relates to a preparation method of sewing thread;
[0049] The preparation method of described sewing thread, comprises the steps:
[0050] (1) Prepare the following components by weight according to the following ratio:
[0051] 35 parts of polypropylene, 6 parts of polyethylene, 6 parts of polyvinyl alcohol, 12 parts of polyacrylamide, 0.8 parts of graphene, 3 parts of bamboo charcoal fiber, 4 parts of additives, 2 parts of emulsifier, 4 parts of additives;
[0052] (2) Weigh the proportioned amount of polyacrylamide and polyvinyl alcohol into the reaction kettle, raise the temperature to 60°C, slowly add graphene, and react at constant temperature for 2 hours to obtain the reaction product a1;
[0053] (3) Weigh the proportioned amount of polypropylene, polyethylene, bamboo charcoal fiber, emulsifier and reaction product a1 and place them in a banbury mixer for 20 minutes of banburying, pulverize the banbury-mixed products, and mix them evenly with a...
Embodiment 3
[0064] This embodiment relates to a preparation method of sewing thread;
[0065] The preparation method of described sewing thread, comprises the steps:
[0066] (1) Prepare the following components by weight according to the following ratio:
[0067] 30 parts of polypropylene, 3 parts of polyethylene, 5 parts of polyvinyl alcohol, 7 parts of polyacrylamide, 0.5 parts of graphene, 3 parts of bamboo charcoal fiber, 2 parts of additives, 1 part of emulsifier, 2 parts of additives;
[0068] (2) Weigh the proportioned amount of polyacrylamide and polyvinyl alcohol into the reaction kettle, raise the temperature to 50°C, slowly add graphene, and react at constant temperature for 2 hours to obtain the reaction product a1;
[0069] (3) Weigh the proportioned amount of polypropylene, polyethylene, bamboo charcoal fiber, emulsifier and reaction product a1, place them in a banbury mixer for 15 minutes, crush the products after banbury mixing, and mix them evenly with additives to obta...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com